| 物理性能 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
|---|---|---|---|---|
| 密度 | - | ASTM D792 | 1.19 | g/cm³ |
| 吸水率 | 23°C,24hr,0.250mm | ASTM D570 | 0.50 | % |
| 机械性能 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
| 耐磨耗性 | 23°C | ASTM D1044 | 23haze | % |
| 光学性能 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
| 光泽度 | 60°,250µm | ASTM D2457 | 161 | - |
| 折射率 | - | ASTM D542 | 1.550 | - |
| 透射率 | 250µm | ASTM D1003 | 92.0 | % |
| 雾度 | 250µm | ASTM D1003 | 0.70 | % |
| 黄度指数 | 250mm | ASTM D1925 | 0.50 | YI |
| UVTransmittance | 250.0µm | - | 89 | % |
| 热性能 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
| 比热 | 60°C | DSC | 1700 | J/kg/°C |
| 100°C | DSC | 1900 | J/kg/°C | |
| 150°C | DSC | 2200 | J/kg/°C | |
| 200°C | DSC | 2400 | J/kg/°C | |
| 250°C | DSC | 2600 | J/kg/°C | |
| 熔融温度 | - | - | 110 | °C |
| 线性热膨胀系数 | MD:23°C,0.250mm | ASTM D696 | 9E-05 | cm/cm/°C |
| 弹性体 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
| 撕裂强度 | 开裂8 | ASTM D1938 | 12 | kN/m |
| 开裂9 | ASTM D1938 | 13 | kN/m | |
| 补充信息 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
| SurfaceEnergy | Total:23°C,250.0µm | ASTM D5946 | 46 | dyne/cm |
| Dispersive:23°C,250.0µm | ASTM D5946 | 39 | dyne/cm | |
| Polar:23°C,250mm | ASTM D5946 | 8 | dyne/cm | |
| 薄膜 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
| 拉伸强度 | TD:屈服,250µm | ASTM D882 | 40.0 | MPa |
| MD:断裂,250µm | ASTM D882 | 59.0 | MPa | |
| TD:断裂,250µm | ASTM D882 | 52.0 | MPa | |
| 伸长率 | MD:屈服,250µm | ASTM D882 | 7.0 | % |
| TD:屈服,250µm | ASTM D882 | 7.0 | % | |
| MD:断裂,250µm | ASTM D882 | 180 | % | |
| 水蒸气透过率 | 23°C,100%RH,250µm | ASTMF1249 | 4.0 | g/m²/24hr |
| 38°C,100%RH,250µm | ASTMF1249 | 11 | g/m²/24hr | |
| 二氧化碳透过率 | 23°C,254.0µm | ASTM D1434 | 150 | cm³·mm/m²/atm/24hr |
| 埃尔曼多夫撕裂强度 | MD:23°C,250.0µm | ASTM D1922 | 5 | N |
| TD:23°C,250.0µm | - | 6 | N | |
| PPTTearResistance | MD:23°C,250.0µm | ASTM D2582 | 42 | N |
| TD:23°C,250.0µm | ASTM D2582 | 56 | N | |
| 撕裂强度 | MD:23°C,250.0µm | ASTM D1938 | 410 | gf |
| TD:23°C,250.0µm | ASTM D1938 | 310 | gf | |
| 薄膜厚度 | - | - | 250 | µm |
| 薄膜穿刺强度 | 250µm | ASTM D3763 | 4.60 | J |
| 割线模量 | MD:250µm | ASTM D882 | 1500 | MPa |
| TD:250µm | ASTM D882 | 1400 | MPa | |
| 拉伸强度 | MD:屈服,250µm | ASTM D882 | 41.0 | MPa |
| 裤型撕裂耐性 | TD:250µm | ISO 6383-1 | 11.0 | N/mm |
| 氧气透过率 | 23°C,250µm,50%RH | ASTM D3985 | 32 | cm³·mm/m²/atm/24hr |
| 伸长率 | TD:断裂 | ASTM D882 | 200 | % |
| 落镖冲击 | -30°C,250µm | ASTM D1709A | 910 | g |
| 23°C,250µm | ASTM D1709A | 880 | g | |
| 裤型撕裂耐性 | MD:250µm | ISO 6383-1 | 11.0 | N/mm |
普拉司网尽最大努力确保此数据的准确性,但是普拉司网对这些数据值不承担任何责任,并强烈建议在最终选择材料前,就数据值与材料供应商进行验证。