物性认证 品名:0 制造商: 0 型号: 0
分享
下载PDF
加入比对
TPU

TPU Texin® 985 U 德国科思创

0
参考价: 0 元/吨
产品描述物性表认证信息替代型号(0)

产品描述

典型应用:
薄膜,密封件,管件,电缆护套,车轮,管道,鞋类,垫圈
颜色:
自然色

物性表

物理性能测试条件测试方法测试结果测试单位
收缩率MD:2.54mmISO 25770.80%
TD:2.54mmASTM D9550.80%
TD:2.54mmISO 25770.80%
密度-ASTM D7921.12g/cm³
-ISO 11831.12g/cm³
收缩率MD:2.54mmASTM D9550.80%
机械性能测试条件测试方法测试结果测试单位
弯曲模量-30°CASTM D79059.0MPa
23°CASTM D79026.9MPa
-30°CISO 17859.0MPa
23°CISO 17826.9MPa
泰伯耐磨性1000Cycles,1000g,H-18转轮ISO 464930.0mg
1000Cycles,1000g,H-18转轮ASTM D104430.0mg
热性能测试条件测试方法测试结果测试单位
脆化温度-ASTM D746<-68.0°C
-ISO 974<-68.0°C
玻璃转化温度-DMA-46.0°C
维卡软化温度-ASTM D1525480.0°C
-ISO 306/5080.0°C
弹性体测试条件测试方法测试结果测试单位
撕裂强度-ASTM D62487.6kN/m
-ISO 34-188kN/m
压缩永久变形23°C,22hr3ASTM D395B16%
23°C,22hrASTM D395B19%
70°C,22hr3ASTM D395B40%
70°C,22hrASTM D395B80%
23°C,22hr3ISO 81516%
23°C,22hrISO 81519%
70°C,22hrISO 81580%
70°C,22hr3ISO 81540%
硬度-ASTM D263245%
拉伸强度50%应变ISO 374.80MPa
50%应变ASTM D4124.80MPa
300%应变ISO 379.70MPa
屈服ASTM D41238.6MPa
屈服ISO 3738.6MPa
伸长率断裂ASTM D412590%
断裂ISO 37590%
拉伸强度100%应变ASTM D4125.50MPa
100%应变ISO 375.50MPa
300%应变ASTM D4129.70MPa
硬度测试条件测试方法测试结果测试单位
硬度邵氏AISO 86885-
邵氏AASTM D224085-
补充信息测试条件测试方法测试结果测试单位
CompressiveLoad20%DeflectionASTM D5754.31MPa
25%DeflectionASTM D5755.52MPa
5%DeflectionASTM D5751.03MPa
50%DeflectionASTM D57516.5MPa
10%DeflectionASTM D5752.07MPa
15%DeflectionASTM D5753.10MPa
2%DeflectionASTM D5750.345MPa
老化测试条件测试方法测试结果测试单位
体积变化100°C,70hr,在ASTM#1油中ASTM D4710.0%
硬度ShoreD,100°C,70hr,inASTM#3OilISO 175-10-
ShoreD,100°C,168hr,inASTM#1OilISO 175-8.0-
ShoreD,100°C,168hr,inASTM#3OilISO 175-13-
空气中硬度(Shore)的变化率ShoreD,23°C,504hr,inReferenceFuelCASTM D471-9.0-
ShoreD,100°C,70hr,inASTM#1OilASTM D471-8.0-
体积变化100°C,336hr,inASTM#1OilISO 1750.0%
100°C,336hr,inASTM#3OilISO 17520%
100°C,504hr,inASTM#1OilISO 1750.0%
23°C,168hr,甲醇ASTM D47144%
23°C,336hr,inReferenceFuelAASTM D4716.0%
23°C,336hr,inReferenceFuelCASTM D47144%
23°C,504hr,inReferenceFuelAASTM D4717.0%
23°C,504hr,inReferenceFuelCASTM D47145%
空气中硬度(Shore)的变化率ShoreD,100°C,168hr,inASTM#1OilASTM D471-8.0-
ShoreD,100°C,168hr,inASTM#3OilASTM D471-13-
ShoreD,100°C,336hr,inASTM#1OilASTM D471-9.0-
ShoreD,100°C,336hr,inASTM#3OilASTM D471-14-
ShoreD,100°C,504hr,inASTM#1OilASTM D471-8.0-
ShoreD,100°C,504hr,inASTM#3OilASTM D471-15-
硬度ShoreD,23°C,70hr,inReferenceFuelA(Isooctane)ISO 175-2.0-
空气中极限伸长率的变化率23°C,70hr,甲醇ASTM D471-7.0%
硬度ShoreD,23°C,336hr,inReferenceFuelA(Isooctane)ISO 1750.0-
ShoreD,23°C,336hr,inReferenceFuelCISO 175-10-
ShoreD,23°C,504hr,inReferenceFuelA(Isooctane)ISO 175-1.0-
ShoreD,23°C,504hr,inReferenceFuelCISO 175-9.0-
空气中极限伸长率的变化率100°C,70hr,在ASTM#3油中ASTM D47114%
100°C,168hr,inASTM#1OilASTM D4717.0%
100°C,168hr,inASTM#3OilASTM D47115%
空气中拉伸强度的变化率300%Strain,100°C,168hr,inASTM#1OilISO 17514%
100°C,168hr,inASTM#3OilISO 175-15%
100%Strain,100°C,168hr,inASTM#3OilISO 175-10%
300%Strain,100°C,168hr,inASTM#3OilISO 17523%
100°C,336hr,inASTM#1OilISO 175-28%
100%Strain,100°C,336hr,inASTM#1OilISO 1751.0%
300%Strain,100°C,336hr,inASTM#1OilISO 17525%
300%Strain,23°C,504hr,inReferenceFuelCISO 175-10%
100°C,70hr,在ASTM#1油中ISO 175-8.0%
100%Strain,100°C,70hr,inASTM#1OilISO 175-15%
300%Strain,100°C,70hr,inASTM#1OilISO 17514%
100°C,70hr,在ASTM#3油中ISO 175-6.0%
100%Strain,100°C,70hr,inASTM#3OilISO 175-20%
300%Strain,100°C,70hr,inASTM#3OilISO 17513%
拉伸应力变化率23°C,504hr,inReferenceFuelA(Isooctane),断裂ISO 1758.0%
23°C,504hr,inReferenceFuelC,断裂ISO 175-3.0%
100°C,70hr,在ASTM#1油中,断裂ISO 17512%
100°C,70hr,在ASTM#3油中,断裂ISO 17514%
空气中拉伸强度的变化率300%Strain,100°C,70hr,inASTM#1OilASTM D47114%
100°C,70hr,在ASTM#3油中ASTM D471-6.0%
100%Strain,100°C,70hr,inASTM#3OilASTM D471-20%
300%Strain,100°C,70hr,inASTM#3OilASTM D47113%
100°C,168hr,inASTM#1OilASTM D471-24%
300%Strain125°C,70hrISO 21620%
125°C,168hrISO 216-58%
100%应变125°C,168hrISO 2164.0%
300%Strain125°C,168hrISO 2168.0%
125°C,336hrISO 216-67%
100%Strain125°C,336hrISO 216-16%
300%Strain125°C,336hrISO 216-8.0%
125°C,504hrISO 216-70%
100%Strain125°C,504hrISO 216-15%
300%Strain125°C,504hrISO 216-10%
23°C,70hr,inReferenceFuelA(Isooctane)ISO 175-4.0%
100%Strain,23°C,70hr,inReferenceFuelA(Isooctane)ISO 17513%
300%Strain,23°C,336hr,inReferenceFuelCASTM D471-14%
100°C,168hr,inASTM#1OilISO 175-24%
100%Strain,100°C,168hr,inASTM#1OilISO 175-20%
100%Strain100°C,168hrISO 216-5.0%
300%Strain100°C,168hrISO 2167.0%
100°C,336hrISO 2163.0%
100%Strain100°C,336hrISO 2162.0%
300%Strain100°C,336hrISO 2168.0%
100°C,504hrISO 216-6.0%
100%Strain100°C,504hrISO 216-10%
300%Strain100°C,504hrISO 21615%
125°C,70hrISO 216-37%
空气中硬度(Shore)的变化率ShoreD,100°C,504hrISO 216-4.0-
ShoreD,125°C,70hrISO 216-5.0-
支撐D,125°C,168hrISO 216-5.0-
ShoreD,125°C,336hrISO 216-7.0-
ShoreD,125°C,504hrISO 216-7.0-
空气中拉伸强度的变化率23°C,70hr,inReferenceFuelA(Isooctane)ASTM D471-4.0%
100°C,504hr,inASTM#3OilASTM D471-44%
100%Strain,100°C,504hr,inASTM#3OilASTM D471-20%
300%Strain,100°C,504hr,inASTM#3OilASTM D471-4.0%
100%Strain,23°C,168hr,inReferenceFuelCISO 175-13%
300%Strain,23°C,168hr,inReferenceFuelCISO 175-4.0%
23°C,336hr,inReferenceFuelA(Isooctane)ISO 17512%
空气中极限伸长率的变化率100°C,70hrASTM D57318%
100°C,168hrASTM D57316%
空气中拉伸强度的变化率100°C,70hrASTM D5734.0%
100%Strain,100°C,70hrASTM D573-10%
体积变化100°C,168hr,inASTM#3OilISO 17519%
100°C,70hr,在ASTM#3油中ASTM D47117%
空气中硬度(Shore)的变化率ShoreD,100°C,70hr,inASTM#3OilASTM D471-10-
硬度ShoreD,100°C,70hr,inASTM#1OilISO 175-8.0-
空气中极限伸长率的变化率100°C,336hr,inASTM#1OilASTM D47112%
100°C,336hr,inASTM#3OilASTM D47122%
100°C,504hr,inASTM#1OilASTM D47117%
100°C,504hr,inASTM#3OilASTM D47129%
拉伸应力变化率23°C,70hr,inReferenceFuelA(Isooctane),断裂ISO 175-14%
空气中极限伸长率的变化率23°C,504hr,inReferenceFuelCASTM D471-3.0%
100°C,70hr,在ASTM#1油中ASTM D47112%
拉伸应力变化率100°C,168hr,inASTM#1Oil,断裂ISO 1757.0%
空气中拉伸强度的变化率300%Strain,23°C,504hr,inReferenceFuelA(Isooctane)ASTM D4714.0%
23°C,504hr,inReferenceFuelCASTM D471-36%
100%Strain,23°C,504hr,inReferenceFuelCASTM D471-15%
300%Strain,23°C,504hr,inReferenceFuelCASTM D471-10%
100°C,70hr,在ASTM#1油中ASTM D471-8.0%
100%Strain,100°C,70hr,inASTM#1OilASTM D471-15%
100%Strain,23°C,70hr,inReferenceFuelA(Isooctane)ASTM D47113%
300%Strain,23°C,70hr,inReferenceFuelA(Isooctane)ASTM D47115%
23°C,70hr,甲醇ASTM D471-38%
100%Strain,23°C,70hr,inReferenceFuelCASTM D471-5.0%
300%Strain,23°C,70hr,inReferenceFuelCASTM D4711.0%
23°C,168hr,inReferenceFuelA(Isooctane)ASTM D4713.0%
300%Strain,100°C,504hr,inASTM#1OilASTM D47123%
100%Strain,23°C,336hr,inReferenceFuelA(Isooctane)ISO 175-4.0%
300%Strain,23°C,336hr,inReferenceFuelA(Isooctane)ISO 1752.0%
23°C,336hr,inReferenceFuelCISO 175-50%
100%Strain,23°C,336hr,inReferenceFuelCISO 175-23%
空气中极限伸长率的变化率100°C,336hrASTM D57324%
100°C,504hrASTM D57316%
125°C,70hrASTM D57319%
体积变化100°C,168hr,inASTM#1OilASTM D4710.0%
100°C,168hr,inASTM#3OilASTM D47119%
100°C,336hr,inASTM#1OilASTM D4710.0%
100°C,336hr,inASTM#3OilASTM D47120%
硬度ShoreD,100°C,336hr,inASTM#1OilISO 175-9.0-
ShoreD,100°C,336hr,inASTM#3OilISO 175-14-
体积变化23°C,168hr,inReferenceFuelAISO 1754.0%
23°C,168hr,甲醇ISO 17544%
23°C,336hr,inReferenceFuelAISO 1756.0%
23°C,336hr,inReferenceFuelCISO 17544%
23°C,504hr,inReferenceFuelAISO 1757.0%
空气中硬度(Shore)的变化率ShoreD,23°C,336hr,inReferenceFuelA(Isooctane)ASTM D4710.0-
ShoreD,23°C,336hr,inReferenceFuelCASTM D471-10-
ShoreD,23°C,504hr,inReferenceFuelA(Isooctane)ASTM D471-1.0-
拉伸应力变化率23°C,70hr,甲醇,断裂ISO 175-7.0%
23°C,168hr,inReferenceFuelA(Isooctane),断裂ISO 1750.0%
23°C,168hr,甲醇,断裂ISO 175-7.0%
23°C,336hr,inReferenceFuelA(Isooctane),断裂ISO 1753.0%
23°C,336hr,inReferenceFuelC,断裂ISO 175-10%
硬度ShoreD,100°C,504hr,inASTM#1OilISO 175-8.0-
ShoreD,100°C,504hr,inASTM#3OilISO 175-15-
体积变化23°C,70hr,inReferenceFuelAASTM D4713.0%
23°C,70hr,甲醇ASTM D47143%
23°C,168hr,inReferenceFuelAASTM D4714.0%
空气中拉伸强度的变化率100°C,336hr,inASTM#3OilISO 175-23%
100%Strain,100°C,336hr,inASTM#3OilISO 175-16%
300%Strain,100°C,336hr,inASTM#3OilISO 17510%
100°C,504hr,inASTM#1OilISO 175-30%
100%Strain,100°C,504hr,inASTM#1OilISO 1753.0%
300%Strain,100°C,504hr,inASTM#1OilISO 17523%
100°C,504hr,inASTM#3OilISO 175-44%
100%Strain,100°C,504hr,inASTM#3OilISO 175-20%
300%Strain,100°C,504hr,inASTM#3OilISO 175-4.0%
空气中极限伸长率的变化率23°C,70hr,inReferenceFuelA(Isooctane)ASTM D471-14%
拉伸应力变化率100°C,168hr,inASTM#3Oil,断裂ISO 17515%
100°C,336hr,inASTM#1Oil,断裂ISO 17512%
100°C,336hr,inASTM#3Oil,断裂ISO 17522%
100°C,504hr,inASTM#1Oil,断裂ISO 17517%
100°C,504hr,inASTM#3Oil,断裂ISO 17529%
空气中拉伸强度的变化率100%Strain,125°C,70hrASTM D5734.0%
空气中极限伸长率的变化率23°C,168hr,inReferenceFuelA(Isooctane)ASTM D4710.0%
23°C,168hr,甲醇ASTM D471-7.0%
23°C,336hr,inReferenceFuelA(Isooctane)ASTM D4713.0%
23°C,336hr,inReferenceFuelCASTM D471-10%
23°C,504hr,inReferenceFuelA(Isooctane)ASTM D4718.0%
空气中拉伸强度的变化率100%Strain,100°C,168hr,inASTM#1OilASTM D471-20%
100%Strain,23°C,504hr,inReferenceFuelCISO 175-15%
300%Strain,23°C,70hr,inReferenceFuelA(Isooctane)ISO 17515%
23°C,70hr,甲醇ISO 175-38%
100%Strain,23°C,70hr,inReferenceFuelCISO 175-5.0%
300%Strain,23°C,70hr,inReferenceFuelCISO 1751.0%
23°C,168hr,inReferenceFuelA(Isooctane)ISO 1753.0%
300%Strain,125°C,70hrASTM D57320%
拉伸应力变化率125°C,70hr,断裂ISO 21619%
125°C,168hr,断裂ISO 21616%
125°C,336hr,断裂ISO 21616%
125°C,504hr,断裂ISO 2162.0%
空气中硬度(Shore)的变化率ShoreD,100°C,70hrASTM D573-4.0-
ShoreD,100°C,168hrASTM D573-5.0-
ShoreD,100°C,336hrASTM D573-4.0-
空气中拉伸强度的变化率100%Strain,23°C,336hr,inReferenceFuelA(Isooctane)ASTM D471-4.0%
300%Strain,23°C,336hr,inReferenceFuelA(Isooctane)ASTM D4712.0%
23°C,336hr,inReferenceFuelCASTM D471-50%
100%Strain,23°C,336hr,inReferenceFuelCASTM D471-23%
300%Strain,23°C,336hr,inReferenceFuelCISO 175-14%
23°C,504hr,inReferenceFuelA(Isooctane)ISO 17513%
空气中极限伸长率的变化率125°C,168hrASTM D57316%
125°C,336hrASTM D57316%
125°C,504hrASTM D5732.0%
拉伸应力变化率100°C,70hr,断裂ISO 21618%
100°C,168hr,断裂ISO 21616%
空气中拉伸强度的变化率300%Strain,100°C,336hr,inASTM#1OilASTM D47125%
100°C,336hr,inASTM#3OilASTM D471-23%
100°C,168hrASTM D5737.0%
100%Strain,100°C,168hrASTM D573-5.0%
300%Strain,100°C,168hrASTM D5737.0%
100°C,336hrASTM D5733.0%
100%Strain,100°C,336hrASTM D5732.0%
300%Strain,100°C,336hrASTM D5738.0%
100°C,504hrASTM D573-6.0%
100%Strain,100°C,504hrASTM D573-10%
300%Strain,100°C,504hrASTM D57315%
125°C,70hrASTM D573-37%
125°C,168hrASTM D573-58%
100%Strain,125°C,168hrASTM D5734.0%
300%Strain,125°C,168hrASTM D5738.0%
125°C,336hrASTM D573-67%
100%Strain,125°C,336hrASTM D573-16%
300%Strain,125°C,336hrASTM D573-8.0%
125°C,504hrASTM D573-70%
100%Strain,125°C,504hrASTM D573-15%
300%Strain,125°C,504hrASTM D573-10%
体积变化100°C,504hr,inASTM#1OilASTM D4710.0%
100°C,504hr,inASTM#3OilASTM D47120%
23°C,70hr,inReferenceFuelAISO 1753.0%
23°C,70hr,甲醇ISO 17543%
23°C,504hr,inReferenceFuelCISO 17545%
100°C,70hr,在ASTM#1油中ISO 1750.0%
100°C,70hr,在ASTM#3油中ISO 17517%
100°C,168hr,inASTM#1OilISO 1750.0%
100°C,504hr,inASTM#3OilISO 17520%
硬度ShoreD,23°C,70hr,inReferenceFuelCISO 175-8.0-
ShoreD,23°C,168hr,inReferenceFuelA(Isooctane)ISO 175-1.0-
ShoreD,23°C,168hr,inReferenceFuelCISO 175-8.0-
空气中硬度(Shore)的变化率ShoreD,23°C,70hr,inReferenceFuelA(Isooctane)ASTM D471-2.0-
ShoreD,23°C,70hr,inReferenceFuelCASTM D471-8.0-
ShoreD,23°C,168hr,inReferenceFuelA(Isooctane)ASTM D471-1.0-
ShoreD,23°C,168hr,inReferenceFuelCASTM D471-8.0-
空气中拉伸强度的变化率300%Strain,100°C,168hr,inASTM#1OilASTM D47114%
100°C,168hr,inASTM#3OilASTM D471-15%
100%Strain,100°C,168hr,inASTM#3OilASTM D471-10%
300%Strain,100°C,168hr,inASTM#3OilASTM D47123%
100°C,336hr,inASTM#1OilASTM D471-28%
100%Strain,100°C,336hr,inASTM#1OilASTM D4711.0%
300%Strain,23°C,504hr,inReferenceFuelA(Isooctane)ISO 1754.0%
23°C,504hr,inReferenceFuelCISO 175-36%
100%Strain,23°C,168hr,inReferenceFuelA(Isooctane)ISO 1750.0%
300%Strain,23°C,168hr,inReferenceFuelA(Isooctane)ISO 1753.0%
23°C,168hr,甲醇ISO 175-34%
23°C,504hr,inReferenceFuelA(Isooctane)ASTM D47113%
100%Strain,23°C,504hr,inReferenceFuelA(Isooctane)ASTM D4717.0%
100%Strain125°C,70hrISO 2164.0%
拉伸应力变化率100°C,336hr,断裂ISO 21624%
100°C,504hr,断裂ISO 21616%
空气中硬度(Shore)的变化率ShoreD,100°C,504hrASTM D573-4.0-
空气中拉伸强度的变化率100%Strain,23°C,168hr,inReferenceFuelA(Isooctane)ASTM D4710.0%
300%Strain,23°C,168hr,inReferenceFuelA(Isooctane)ASTM D4713.0%
23°C,168hr,甲醇ASTM D471-34%
100%Strain,23°C,168hr,inReferenceFuelCASTM D471-13%
300%Strain,23°C,168hr,inReferenceFuelCASTM D471-4.0%
23°C,336hr,inReferenceFuelA(Isooctane)ASTM D47112%
100%Strain,23°C,504hr,inReferenceFuelA(Isooctane)ISO 1757.0%
空气中硬度(Shore)的变化率ShoreD,125°C,70hrASTM D573-5.0-
支撐D,125°C,168hrASTM D573-5.0-
ShoreD,125°C,336hrASTM D573-7.0-
ShoreD,125°C,504hrASTM D573-7.0-
ShoreD,100°C,70hrISO 216-4.0-
ShoreD,100°C,168hrISO 216-5.0-
ShoreD,100°C,336hrISO 216-4.0-
空气中拉伸强度的变化率100%Strain,100°C,336hr,inASTM#3OilASTM D471-16%
300%Strain,100°C,336hr,inASTM#3OilASTM D47110%
100°C,504hr,inASTM#1OilASTM D471-30%
100%Strain,100°C,504hr,inASTM#1OilASTM D4713.0%
300%Strain,100°C,70hrASTM D5730.0%
100°C,70hrISO 2164.0%
100%Strain100°C,70hrISO 216-10%
300%Strain100°C,70hrISO 2160.0%
100°C,168hrISO 2167.0%

【免责声明】

普拉司网尽最大努力确保此数据的准确性,但是普拉司网对这些数据值不承担任何责任,并强烈建议在最终选择材料前,就数据值与材料供应商进行验证。