| 物理性能 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
|---|---|---|---|---|
| 收缩率 | TD:2.54mm | ISO 2577 | 0.80 | % |
| MD:2.54mm | ISO 2577 | 0.80 | % | |
| MD:2.54mm | ASTM D955 | 0.80 | % | |
| TD:2.54mm | ASTM D955 | 0.80 | % | |
| 密度 | - | ASTM D792 | 1.12 | g/cm³ |
| - | ISO 1183 | 1.12 | g/cm³ | |
| 机械性能 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
| 弯曲模量 | -30°C | ASTM D790 | 59.0 | MPa |
| 23°C | ASTM D790 | 26.9 | MPa | |
| -30°C | ISO 178 | 59.0 | MPa | |
| 23°C | ISO 178 | 26.9 | MPa | |
| 泰伯耐磨性 | 1000Cycles,1000g,H-18转轮 | ISO 4649 | 30.0 | mg |
| 1000Cycles,1000g,H-18转轮 | ASTM D1044 | 30.0 | mg | |
| 热性能 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
| 维卡软化温度 | - | ASTM D15254 | 80.0 | °C |
| - | ISO 306/50 | 80.0 | °C | |
| 脆化温度 | - | ASTM D746 | <-68.0 | °C |
| - | ISO 974 | <-68.0 | °C | |
| 玻璃转化温度 | - | DMA | -46.0 | °C |
| 弹性体 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
| 拉伸强度 | 50%应变 | ISO 37 | 4.80 | MPa |
| 50%应变 | ASTM D412 | 4.80 | MPa | |
| 100%应变 | ASTM D412 | 5.50 | MPa | |
| 100%应变 | ISO 37 | 5.50 | MPa | |
| 300%应变 | ASTM D412 | 9.70 | MPa | |
| 300%应变 | ISO 37 | 9.70 | MPa | |
| 屈服 | ASTM D412 | 38.6 | MPa | |
| 屈服 | ISO 37 | 38.6 | MPa | |
| 伸长率 | 断裂 | ASTM D412 | 590 | % |
| 断裂 | ISO 37 | 590 | % | |
| 撕裂强度 | - | ASTM D624 | 87.6 | kN/m |
| - | ISO 34-1 | 88 | kN/m | |
| 压缩永久变形 | 23°C,22hr3 | ASTM D395B | 16 | % |
| 23°C,22hr | ASTM D395B | 19 | % | |
| 70°C,22hr3 | ASTM D395B | 40 | % | |
| 70°C,22hr | ASTM D395B | 80 | % | |
| 70°C,22hr | ISO 815 | 80 | % | |
| 硬度 | - | ASTM D2632 | 45 | % |
| 压缩永久变形 | 23°C,22hr3 | ISO 815 | 16 | % |
| 23°C,22hr | ISO 815 | 19 | % | |
| 70°C,22hr3 | ISO 815 | 40 | % | |
| 硬度 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
| 硬度 | 邵氏A | ASTM D2240 | 85 | - |
| 邵氏A | ISO 868 | 85 | - | |
| 补充信息 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
| CompressiveLoad | 10%Deflection | ASTM D575 | 2.07 | MPa |
| 15%Deflection | ASTM D575 | 3.10 | MPa | |
| 2%Deflection | ASTM D575 | 0.345 | MPa | |
| 20%Deflection | ASTM D575 | 4.31 | MPa | |
| 25%Deflection | ASTM D575 | 5.52 | MPa | |
| 5%Deflection | ASTM D575 | 1.03 | MPa | |
| 50%Deflection | ASTM D575 | 16.5 | MPa | |
| 老化 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
| 拉伸应力变化率 | 100°C,504hr,inASTM#1Oil,断裂 | ISO 175 | 17 | % |
| 100°C,504hr,inASTM#3Oil,断裂 | ISO 175 | 29 | % | |
| 空气中硬度(Shore)的变化率 | ShoreD,23°C,70hr,inReferenceFuelA(Isooctane) | ASTM D471 | -2.0 | - |
| ShoreD,23°C,70hr,inReferenceFuelC | ASTM D471 | -8.0 | - | |
| ShoreD,23°C,168hr,inReferenceFuelA(Isooctane) | ASTM D471 | -1.0 | - | |
| 体积变化 | 100°C,504hr,inASTM#3Oil | ISO 175 | 20 | % |
| 100°C,336hr,inASTM#3Oil | ISO 175 | 20 | % | |
| 100°C,504hr,inASTM#1Oil | ISO 175 | 0.0 | % | |
| 空气中极限伸长率的变化率 | 100°C,504hr,inASTM#3Oil | ASTM D471 | 29 | % |
| 体积变化 | 23°C,504hr,inReferenceFuelC | ASTM D471 | 45 | % |
| 100°C,70hr,在ASTM#1油中 | ASTM D471 | 0.0 | % | |
| 100°C,70hr,在ASTM#3油中 | ASTM D471 | 17 | % | |
| 100°C,168hr,inASTM#1Oil | ASTM D471 | 0.0 | % | |
| 空气中拉伸强度的变化率 | 300%Strain,100°C,504hr,inASTM#3Oil | ISO 175 | -4.0 | % |
| 空气中极限伸长率的变化率 | 23°C,70hr,inReferenceFuelA(Isooctane) | ASTM D471 | -14 | % |
| 硬度 | ShoreD,23°C,70hr,inReferenceFuelC | ISO 175 | -8.0 | - |
| ShoreD,23°C,168hr,inReferenceFuelA(Isooctane) | ISO 175 | -1.0 | - | |
| ShoreD,23°C,168hr,inReferenceFuelC | ISO 175 | -8.0 | - | |
| ShoreD,23°C,336hr,inReferenceFuelA(Isooctane) | ISO 175 | 0.0 | - | |
| ShoreD,23°C,336hr,inReferenceFuelC | ISO 175 | -10 | - | |
| ShoreD,23°C,504hr,inReferenceFuelA(Isooctane) | ISO 175 | -1.0 | - | |
| 空气中拉伸强度的变化率 | 100°C,70hr | ASTM D573 | 4.0 | % |
| 空气中极限伸长率的变化率 | 100°C,504hr | ASTM D573 | 16 | % |
| 空气中拉伸强度的变化率 | 300%Strain,23°C,336hr,inReferenceFuelC | ISO 175 | -14 | % |
| 23°C,504hr,inReferenceFuelA(Isooctane) | ISO 175 | 13 | % | |
| 100%Strain,23°C,504hr,inReferenceFuelA(Isooctane) | ISO 175 | 7.0 | % | |
| 300%Strain,23°C,504hr,inReferenceFuelA(Isooctane) | ISO 175 | 4.0 | % | |
| 23°C,504hr,inReferenceFuelC | ISO 175 | -36 | % | |
| 100%Strain,23°C,504hr,inReferenceFuelC | ISO 175 | -15 | % | |
| 100°C,168hr,inASTM#3Oil | ISO 175 | -15 | % | |
| 100%Strain100°C,336hr | ISO 216 | 2.0 | % | |
| 300%Strain100°C,336hr | ISO 216 | 8.0 | % | |
| 100°C,504hr | ISO 216 | -6.0 | % | |
| 100%Strain100°C,504hr | ISO 216 | -10 | % | |
| 300%Strain100°C,504hr | ISO 216 | 15 | % | |
| 100%Strain,100°C,168hr,inASTM#1Oil | ASTM D471 | -20 | % | |
| 300%Strain,100°C,168hr,inASTM#1Oil | ASTM D471 | 14 | % | |
| 100°C,168hr,inASTM#3Oil | ASTM D471 | -15 | % | |
| 100%Strain,100°C,168hr,inASTM#3Oil | ASTM D471 | -10 | % | |
| 300%Strain,100°C,168hr,inASTM#3Oil | ASTM D471 | 23 | % | |
| 300%Strain,23°C,504hr,inReferenceFuelC | ASTM D471 | -10 | % | |
| 100°C,70hr,在ASTM#1油中 | ASTM D471 | -8.0 | % | |
| 100%Strain,100°C,70hr,inASTM#1Oil | ASTM D471 | -15 | % | |
| 300%Strain,100°C,70hr,inASTM#1Oil | ASTM D471 | 14 | % | |
| 100°C,70hr,在ASTM#3油中 | ASTM D471 | -6.0 | % | |
| 100%Strain,100°C,70hr,inASTM#3Oil | ASTM D471 | -20 | % | |
| 300%Strain,100°C,70hr,inASTM#3Oil | ASTM D471 | 13 | % | |
| 100°C,168hr,inASTM#1Oil | ASTM D471 | -24 | % | |
| 300%Strain,100°C,504hr | ASTM D573 | 15 | % | |
| 空气中极限伸长率的变化率 | 100°C,336hr,inASTM#1Oil | ASTM D471 | 12 | % |
| 100°C,336hr,inASTM#3Oil | ASTM D471 | 22 | % | |
| 100°C,504hr,inASTM#1Oil | ASTM D471 | 17 | % | |
| 体积变化 | 23°C,70hr,inReferenceFuelA | ASTM D471 | 3.0 | % |
| 拉伸应力变化率 | 100°C,70hr,在ASTM#3油中,断裂 | ISO 175 | 14 | % |
| 100°C,168hr,inASTM#1Oil,断裂 | ISO 175 | 7.0 | % | |
| 100°C,168hr,inASTM#3Oil,断裂 | ISO 175 | 15 | % | |
| 100°C,336hr,inASTM#1Oil,断裂 | ISO 175 | 12 | % | |
| 100°C,336hr,inASTM#3Oil,断裂 | ISO 175 | 22 | % | |
| 23°C,70hr,inReferenceFuelA(Isooctane),断裂 | ISO 175 | -14 | % | |
| 23°C,70hr,甲醇,断裂 | ISO 175 | -7.0 | % | |
| 23°C,168hr,inReferenceFuelA(Isooctane),断裂 | ISO 175 | 0.0 | % | |
| 23°C,168hr,甲醇,断裂 | ISO 175 | -7.0 | % | |
| 23°C,336hr,inReferenceFuelA(Isooctane),断裂 | ISO 175 | 3.0 | % | |
| 23°C,336hr,inReferenceFuelC,断裂 | ISO 175 | -10 | % | |
| 23°C,504hr,inReferenceFuelA(Isooctane),断裂 | ISO 175 | 8.0 | % | |
| 23°C,504hr,inReferenceFuelC,断裂 | ISO 175 | -3.0 | % | |
| 100°C,70hr,在ASTM#1油中,断裂 | ISO 175 | 12 | % | |
| 体积变化 | 23°C,70hr,甲醇 | ASTM D471 | 43 | % |
| 23°C,168hr,inReferenceFuelA | ASTM D471 | 4.0 | % | |
| 23°C,168hr,甲醇 | ASTM D471 | 44 | % | |
| 23°C,336hr,inReferenceFuelA | ASTM D471 | 6.0 | % | |
| 23°C,336hr,inReferenceFuelC | ASTM D471 | 44 | % | |
| 23°C,504hr,inReferenceFuelA | ASTM D471 | 7.0 | % | |
| 空气中拉伸强度的变化率 | 100%Strain,100°C,504hr,inASTM#1Oil | ISO 175 | -3.0 | % |
| 300%Strain,100°C,504hr,inASTM#1Oil | ISO 175 | 23 | % | |
| 100°C,504hr,inASTM#3Oil | ISO 175 | -44 | % | |
| 100%Strain,100°C,504hr,inASTM#3Oil | ISO 175 | -20 | % | |
| 23°C,70hr,inReferenceFuelA(Isooctane) | ISO 175 | -4.0 | % | |
| 100%Strain,23°C,70hr,inReferenceFuelA(Isooctane) | ISO 175 | 13 | % | |
| 300%Strain,23°C,70hr,inReferenceFuelA(Isooctane) | ISO 175 | 15 | % | |
| 23°C,336hr,inReferenceFuelA(Isooctane) | ISO 175 | 12 | % | |
| 空气中极限伸长率的变化率 | 125°C,70hr | ASTM D573 | 19 | % |
| 125°C,168hr | ASTM D573 | 16 | % | |
| 125°C,336hr | ASTM D573 | 16 | % | |
| 125°C,504hr | ASTM D573 | 2.0 | % | |
| 拉伸应力变化率 | 100°C,70hr,断裂 | ISO 216 | 18 | % |
| 100°C,168hr,断裂 | ISO 216 | 16 | % | |
| 100°C,336hr,断裂 | ISO 216 | 24 | % | |
| 空气中硬度(Shore)的变化率 | ShoreD,125°C,70hr | ASTM D573 | -5.0 | - |
| 支撐D,125°C,168hr | ASTM D573 | -5.0 | - | |
| ShoreD,125°C,336hr | ASTM D573 | -7.0 | - | |
| 空气中拉伸强度的变化率 | 100%Strain,23°C,336hr,inReferenceFuelA(Isooctane) | ISO 175 | -4.0 | % |
| 300%Strain,23°C,336hr,inReferenceFuelA(Isooctane) | ISO 175 | 2.0 | % | |
| 23°C,336hr,inReferenceFuelC | ISO 175 | -50 | % | |
| 100%Strain,23°C,336hr,inReferenceFuelC | ISO 175 | -23 | % | |
| 硬度 | ShoreD,23°C,504hr,inReferenceFuelC | ISO 175 | -9.0 | - |
| ShoreD,100°C,70hr,inASTM#1Oil | ISO 175 | -8.0 | - | |
| ShoreD,100°C,70hr,inASTM#3Oil | ISO 175 | -10 | - | |
| ShoreD,100°C,168hr,inASTM#1Oil | ISO 175 | -8.0 | - | |
| ShoreD,100°C,168hr,inASTM#3Oil | ISO 175 | -13 | - | |
| 空气中拉伸强度的变化率 | 125°C,70hr | ISO 216 | -37 | % |
| 100%Strain125°C,70hr | ISO 216 | 4.0 | % | |
| 300%Strain125°C,70hr | ISO 216 | 20 | % | |
| 100°C,70hr,在ASTM#1油中 | ISO 175 | -8.0 | % | |
| 100%Strain,100°C,70hr,inASTM#1Oil | ISO 175 | -15 | % | |
| 300%Strain,100°C,70hr,inASTM#1Oil | ISO 175 | 14 | % | |
| 100°C,70hr,在ASTM#3油中 | ISO 175 | -6.0 | % | |
| 100%Strain,100°C,70hr,inASTM#3Oil | ISO 175 | -20 | % | |
| 300%Strain,100°C,70hr,inASTM#3Oil | ISO 175 | 13 | % | |
| 100°C,168hr,inASTM#1Oil | ISO 175 | -24 | % | |
| 100%Strain,100°C,168hr,inASTM#1Oil | ISO 175 | -20 | % | |
| 300%Strain,100°C,168hr,inASTM#1Oil | ISO 175 | 14 | % | |
| 体积变化 | 23°C,70hr,甲醇 | ISO 175 | 43 | % |
| 23°C,168hr,inReferenceFuelA | ISO 175 | 4.0 | % | |
| 23°C,168hr,甲醇 | ISO 175 | 44 | % | |
| 23°C,336hr,inReferenceFuelA | ISO 175 | 6.0 | % | |
| 23°C,336hr,inReferenceFuelC | ISO 175 | 44 | % | |
| 23°C,504hr,inReferenceFuelA | ISO 175 | 7.0 | % | |
| 23°C,504hr,inReferenceFuelC | ISO 175 | 45 | % | |
| 100°C,70hr,在ASTM#1油中 | ISO 175 | 0.0 | % | |
| 100°C,70hr,在ASTM#3油中 | ISO 175 | 17 | % | |
| 100°C,168hr,inASTM#1Oil | ISO 175 | 0.0 | % | |
| 100°C,168hr,inASTM#3Oil | ISO 175 | 19 | % | |
| 100°C,336hr,inASTM#1Oil | ISO 175 | 0.0 | % | |
| 空气中拉伸强度的变化率 | 100%Strain,100°C,70hr | ASTM D573 | -10 | % |
| 300%Strain,100°C,70hr | ASTM D573 | 0.0 | % | |
| 100°C,168hr | ASTM D573 | 7.0 | % | |
| 100%Strain,100°C,168hr | ASTM D573 | -5.0 | % | |
| 300%Strain,100°C,168hr | ASTM D573 | 7.0 | % | |
| 100°C,336hr | ASTM D573 | 3.0 | % | |
| 100%Strain,100°C,336hr | ASTM D573 | 2.0 | % | |
| 300%Strain,100°C,336hr | ASTM D573 | 8.0 | % | |
| 100°C,504hr | ASTM D573 | -6.0 | % | |
| 100%Strain,100°C,504hr | ASTM D573 | -10 | % | |
| 23°C,504hr,inReferenceFuelC | ASTM D471 | -36 | % | |
| 100%Strain,23°C,504hr,inReferenceFuelC | ASTM D471 | -15 | % | |
| 空气中硬度(Shore)的变化率 | ShoreD,23°C,168hr,inReferenceFuelC | ASTM D471 | -8.0 | - |
| ShoreD,23°C,336hr,inReferenceFuelA(Isooctane) | ASTM D471 | 0.0 | - | |
| ShoreD,23°C,336hr,inReferenceFuelC | ASTM D471 | -10 | - | |
| 空气中拉伸强度的变化率 | 100%Strain,100°C,168hr,inASTM#3Oil | ISO 175 | -10 | % |
| 300%Strain,100°C,168hr,inASTM#3Oil | ISO 175 | 23 | % | |
| 100°C,336hr,inASTM#1Oil | ISO 175 | -28 | % | |
| 100%Strain,100°C,336hr,inASTM#1Oil | ISO 175 | 1.0 | % | |
| 300%Strain,100°C,336hr,inASTM#1Oil | ISO 175 | 25 | % | |
| 100°C,336hr,inASTM#3Oil | ISO 175 | -23 | % | |
| 100%Strain,100°C,336hr,inASTM#3Oil | ISO 175 | -16 | % | |
| 300%Strain,100°C,336hr,inASTM#3Oil | ISO 175 | 10 | % | |
| 100%Strain,23°C,336hr,inReferenceFuelA(Isooctane) | ASTM D471 | -4.0 | % | |
| 300%Strain,23°C,336hr,inReferenceFuelA(Isooctane) | ASTM D471 | 2.0 | % | |
| 23°C,336hr,inReferenceFuelC | ASTM D471 | -50 | % | |
| 100%Strain,23°C,336hr,inReferenceFuelC | ASTM D471 | -23 | % | |
| 300%Strain,23°C,336hr,inReferenceFuelC | ASTM D471 | -14 | % | |
| 23°C,504hr,inReferenceFuelA(Isooctane) | ASTM D471 | 13 | % | |
| 100%Strain,23°C,504hr,inReferenceFuelA(Isooctane) | ASTM D471 | 7.0 | % | |
| 300%Strain,23°C,504hr,inReferenceFuelA(Isooctane) | ASTM D471 | 4.0 | % | |
| 300%Strain,100°C,336hr,inASTM#3Oil | ASTM D471 | 10 | % | |
| 100°C,504hr,inASTM#1Oil | ASTM D471 | -30 | % | |
| 100%Strain,100°C,504hr,inASTM#1Oil | ASTM D471 | -3.0 | % | |
| 300%Strain,100°C,504hr,inASTM#1Oil | ASTM D471 | 23 | % | |
| 23°C,70hr,inReferenceFuelA(Isooctane) | ASTM D471 | -4.0 | % | |
| 23°C,70hr,甲醇 | ISO 175 | -38 | % | |
| 100%Strain,23°C,70hr,inReferenceFuelC | ISO 175 | -5.0 | % | |
| 300%Strain,23°C,70hr,inReferenceFuelC | ISO 175 | 1.0 | % | |
| 23°C,168hr,inReferenceFuelA(Isooctane) | ISO 175 | 3.0 | % | |
| 100%Strain,23°C,168hr,inReferenceFuelA(Isooctane) | ISO 175 | 0.0 | % | |
| 300%Strain,23°C,168hr,inReferenceFuelA(Isooctane) | ISO 175 | 3.0 | % | |
| 23°C,168hr,甲醇 | ISO 175 | -34 | % | |
| 100%Strain,23°C,168hr,inReferenceFuelC | ISO 175 | -13 | % | |
| 300%Strain,23°C,168hr,inReferenceFuelC | ISO 175 | -4.0 | % | |
| 100°C,336hr,inASTM#1Oil | ASTM D471 | -28 | % | |
| 100%Strain,100°C,336hr,inASTM#1Oil | ASTM D471 | 1.0 | % | |
| 拉伸应力变化率 | 125°C,336hr,断裂 | ISO 216 | 16 | % |
| 125°C,504hr,断裂 | ISO 216 | 2.0 | % | |
| 空气中硬度(Shore)的变化率 | ShoreD,100°C,70hr | ASTM D573 | -4.0 | - |
| ShoreD,100°C,168hr | ASTM D573 | -5.0 | - | |
| ShoreD,100°C,336hr | ASTM D573 | -4.0 | - | |
| ShoreD,100°C,504hr | ASTM D573 | -4.0 | - | |
| 空气中拉伸强度的变化率 | 125°C,70hr | ASTM D573 | -37 | % |
| 100%Strain,125°C,70hr | ASTM D573 | 4.0 | % | |
| 300%Strain,125°C,70hr | ASTM D573 | 20 | % | |
| 125°C,168hr | ASTM D573 | -58 | % | |
| 100%Strain,125°C,168hr | ASTM D573 | 4.0 | % | |
| 300%Strain,125°C,168hr | ASTM D573 | 8.0 | % | |
| 125°C,336hr | ASTM D573 | -67 | % | |
| 125°C,504hr | ASTM D573 | -70 | % | |
| 100%Strain,125°C,504hr | ASTM D573 | -15 | % | |
| 300%Strain,125°C,504hr | ASTM D573 | -10 | % | |
| 100°C,70hr | ISO 216 | 4.0 | % | |
| 100%Strain100°C,70hr | ISO 216 | -10 | % | |
| 300%Strain100°C,70hr | ISO 216 | 0.0 | % | |
| 100°C,168hr | ISO 216 | 7.0 | % | |
| 空气中极限伸长率的变化率 | 23°C,336hr,inReferenceFuelC | ASTM D471 | -10 | % |
| 23°C,504hr,inReferenceFuelA(Isooctane) | ASTM D471 | 8.0 | % | |
| 23°C,504hr,inReferenceFuelC | ASTM D471 | -3.0 | % | |
| 100°C,70hr,在ASTM#1油中 | ASTM D471 | 12 | % | |
| 100°C,70hr,在ASTM#3油中 | ASTM D471 | 14 | % | |
| 100°C,168hr,inASTM#1Oil | ASTM D471 | 7.0 | % | |
| 100°C,168hr,inASTM#3Oil | ASTM D471 | 15 | % | |
| 硬度 | ShoreD,100°C,336hr,inASTM#1Oil | ISO 175 | -9.0 | - |
| ShoreD,100°C,336hr,inASTM#3Oil | ISO 175 | -14 | - | |
| ShoreD,100°C,504hr,inASTM#1Oil | ISO 175 | -82 | - | |
| ShoreD,100°C,504hr,inASTM#3Oil | ISO 175 | -15 | - | |
| 空气中极限伸长率的变化率 | 23°C,70hr,甲醇 | ASTM D471 | -7.0 | % |
| 23°C,168hr,inReferenceFuelA(Isooctane) | ASTM D471 | 0.0 | % | |
| 23°C,168hr,甲醇 | ASTM D471 | -7.0 | % | |
| 23°C,336hr,inReferenceFuelA(Isooctane) | ASTM D471 | 3.0 | % | |
| 体积变化 | 100°C,168hr,inASTM#3Oil | ASTM D471 | 19 | % |
| 100°C,336hr,inASTM#1Oil | ASTM D471 | 0.0 | % | |
| 100°C,336hr,inASTM#3Oil | ASTM D471 | 20 | % | |
| 100°C,504hr,inASTM#1Oil | ASTM D471 | 0.0 | % | |
| 100°C,504hr,inASTM#3Oil | ASTM D471 | 20 | % | |
| 23°C,70hr,inReferenceFuelA | ISO 175 | 3.0 | % | |
| 空气中硬度(Shore)的变化率 | ShoreD,23°C,504hr,inReferenceFuelA(Isooctane) | ASTM D471 | -1.0 | - |
| ShoreD,23°C,504hr,inReferenceFuelC | ASTM D471 | -9.0 | - | |
| ShoreD,100°C,70hr,inASTM#1Oil | ASTM D471 | -8.0 | - | |
| ShoreD,100°C,70hr,inASTM#3Oil | ASTM D471 | -10 | - | |
| ShoreD,100°C,168hr,inASTM#1Oil | ASTM D471 | -8.0 | - | |
| ShoreD,100°C,168hr,inASTM#3Oil | ASTM D471 | -13 | - | |
| ShoreD,100°C,336hr,inASTM#1Oil | ASTM D471 | -9.0 | - | |
| ShoreD,100°C,336hr,inASTM#3Oil | ASTM D471 | -14 | - | |
| ShoreD,100°C,504hr,inASTM#1Oil | ASTM D471 | -82 | - | |
| ShoreD,100°C,504hr,inASTM#3Oil | ASTM D471 | -15 | - | |
| 硬度 | ShoreD,23°C,70hr,inReferenceFuelA(Isooctane) | ISO 175 | -2.0 | - |
| 空气中拉伸强度的变化率 | 100°C,504hr,inASTM#1Oil | ISO 175 | -30 | % |
| 拉伸应力变化率 | 100°C,504hr,断裂 | ISO 216 | 16 | % |
| 125°C,70hr,断裂 | ISO 216 | 19 | % | |
| 空气中拉伸强度的变化率 | 300%Strain,23°C,168hr,inReferenceFuelC | ASTM D471 | -4.0 | % |
| 23°C,336hr,inReferenceFuelA(Isooctane) | ASTM D471 | 12 | % | |
| 100°C,504hr,inASTM#3Oil | ASTM D471 | -44 | % | |
| 100%Strain,100°C,504hr,inASTM#3Oil | ASTM D471 | -20 | % | |
| 300%Strain,100°C,504hr,inASTM#3Oil | ASTM D471 | -4.0 | % | |
| 125°C,168hr | ISO 216 | -58 | % | |
| 100%应变125°C,168hr | ISO 216 | 4.0 | % | |
| 空气中硬度(Shore)的变化率 | ShoreD,125°C,504hr | ASTM D573 | -7.0 | - |
| ShoreD,100°C,70hr | ISO 216 | -4.0 | - | |
| ShoreD,100°C,168hr | ISO 216 | -5.0 | - | |
| ShoreD,100°C,336hr | ISO 216 | -4.0 | - | |
| ShoreD,100°C,504hr | ISO 216 | -4.0 | - | |
| ShoreD,125°C,70hr | ISO 216 | -5.0 | - | |
| 支撐D,125°C,168hr | ISO 216 | -5.0 | - | |
| ShoreD,125°C,336hr | ISO 216 | -7.0 | - | |
| ShoreD,125°C,504hr | ISO 216 | -7.0 | - | |
| 空气中拉伸强度的变化率 | 300%Strain,100°C,336hr,inASTM#1Oil | ASTM D471 | 25 | % |
| 100°C,336hr,inASTM#3Oil | ASTM D471 | -23 | % | |
| 100%Strain,100°C,336hr,inASTM#3Oil | ASTM D471 | -16 | % | |
| 300%Strain125°C,168hr | ISO 216 | 8.0 | % | |
| 125°C,336hr | ISO 216 | -67 | % | |
| 100%Strain125°C,336hr | ISO 216 | -16 | % | |
| 300%Strain125°C,336hr | ISO 216 | -8.0 | % | |
| 125°C,504hr | ISO 216 | -70 | % | |
| 100%Strain125°C,504hr | ISO 216 | -15 | % | |
| 300%Strain125°C,504hr | ISO 216 | -10 | % | |
| 空气中极限伸长率的变化率 | 100°C,70hr | ASTM D573 | 18 | % |
| 100°C,168hr | ASTM D573 | 16 | % | |
| 100°C,336hr | ASTM D573 | 24 | % | |
| 拉伸应力变化率 | 125°C,168hr,断裂 | ISO 216 | 16 | % |
| 空气中拉伸强度的变化率 | 100%Strain,125°C,336hr | ASTM D573 | -16 | % |
| 300%Strain,125°C,336hr | ASTM D573 | -8.0 | % | |
| 100%Strain,23°C,70hr,inReferenceFuelA(Isooctane) | ASTM D471 | 13 | % | |
| 300%Strain,23°C,70hr,inReferenceFuelA(Isooctane) | ASTM D471 | 15 | % | |
| 23°C,70hr,甲醇 | ASTM D471 | -38 | % | |
| 100%Strain,23°C,70hr,inReferenceFuelC | ASTM D471 | -5.0 | % | |
| 300%Strain,23°C,70hr,inReferenceFuelC | ASTM D471 | 1.0 | % | |
| 23°C,168hr,inReferenceFuelA(Isooctane) | ASTM D471 | 3.0 | % | |
| 100%Strain,23°C,168hr,inReferenceFuelA(Isooctane) | ASTM D471 | 0.0 | % | |
| 300%Strain,23°C,168hr,inReferenceFuelA(Isooctane) | ASTM D471 | 3.0 | % | |
| 23°C,168hr,甲醇 | ASTM D471 | -34 | % | |
| 100%Strain,23°C,168hr,inReferenceFuelC | ASTM D471 | -13 | % | |
| 300%Strain,23°C,504hr,inReferenceFuelC | ISO 175 | -10 | % | |
| 100%Strain100°C,168hr | ISO 216 | -5.0 | % | |
| 300%Strain100°C,168hr | ISO 216 | 7.0 | % | |
| 100°C,336hr | ISO 216 | 3.0 | % |
普拉司网尽最大努力确保此数据的准确性,但是普拉司网对这些数据值不承担任何责任,并强烈建议在最终选择材料前,就数据值与材料供应商进行验证。