| 物理性能 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
|---|---|---|---|---|
| 耐清洗剂性 | - | UL 749 | f3 | - |
| 密度 | - | ASTM D792 | 0.968 | g/cm³ |
| - | ISO 1183 | 0.970 | g/cm³ | |
| 耐清洗剂性 | - | UL 2157 | f4 | - |
| 热性能 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
| 脆化温度 | - | ASTM D746 | -60.0 | °C |
| - | ISO 812 | -60.0 | °C | |
| RTI Elec | - | UL 746 | 100 | °C |
| RTI Str | 1.0mm | UL 746 | 90.0 | °C |
| 1.5mm | UL 746 | 95.0 | °C | |
| 3.0mm | UL 746 | 100 | °C | |
| 电气性能 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
| 介电强度 | 23°C,2.00mm | ASTM D149 | 29 | kV/mm |
| 介电常数 | 23°C,1.98mm | ASTM D150 | 2.30 | - |
| 高电压电弧起痕速率 | HVTR | UL 746 | PLC 1 | - |
| 热丝引燃 | 1.5mm | UL 746 | PLC 3 | - |
| 3.0mm | UL 746 | PLC 2 | - | |
| 介电常数 | 23°C,1.98mm | IEC 60250 | 2.30 | - |
| 相比漏电起痕指数 | CTI | UL 746 | PLC 0 | - |
| 高电弧燃烧指数 | HAI | UL 746 | PLC 0 | - |
| 弹性体 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
| 撕裂强度 | 23°C,横向流量 | ASTM D624 | 16.0 | kN/m |
| 23°C,Across Flow (横向) | ISO 34-1 | 16 | kN/m | |
| 压缩永久变形 | 70°C,22hr | ASTM D395B | 22 | % |
| 伸长率 | 断裂,23°C,横向 | ASTM D412 | 400 | % |
| 拉伸应力 | 100%应变,23°C,横向流量 | ASTM D412 | 2.10 | MPa |
| 压缩永久变形 | 125°C,70hr | ASTM D395B | 38 | % |
| 70°C,22hr | ISO 815 | 22 | % | |
| 125°C,70hr | ISO 815 | 38 | % | |
| 伸长率 | 断裂,23°C,横向 | ISO 37 | 400 | % |
| 拉伸应力 | 100%应变,23°C,横向流量 | ISO 37 | 2.10 | MPa |
| 拉伸强度 | 断裂,23°C,横向流量 | ASTM D412 | 5.20 | MPa |
| Break,23°C | ISO 37 | 5.20 | MPa | |
| 硬度 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
| 硬度 | 邵氏A,15秒,23°C | ISO 868 | 59 | - |
| 可燃性 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
| UL阻燃等级 | 1.0mm | UL 94 | HB | - |
| 1.5mm | UL 94 | HB | - | |
| 3.0mm | UL 94 | HB | - | |
| 老化 | 测试条件 | 测试方法 | 测试结果 | 测试单位 |
| 空气中硬度(Shore)的变化率 | ShoreA,23°C,166hr,inPyridine | ASTM D471 | 2.0 | - |
| ShoreA,23°C,166hr,inReferenceFuelA(Isooctane) | ASTM D471 | -13 | - | |
| ShoreA,23°C,168hr,inEthanol,95% | ASTM D471 | 0.0 | - | |
| ShoreA,23°C,168hr,inHydrochloricAcid,10% | ASTM D471 | 1.0 | - | |
| ShoreA,23°C,166hr,inn-Hexane | ASTM D471 | -9.0 | - | |
| ShoreA,23°C,166hr,inn-ButylAcetate | ASTM D471 | -1.0 | - | |
| 拉伸应力变化率 | 125°C,168hr,inIRM903Oil,断裂 | ISO 1817 | -56 | % |
| 125°C,168hr,inASTM#1Oil,断裂 | ISO 1817 | -43 | % | |
| 125°C,166hr,inUcon®CC732,断裂 | ISO 1817 | -9.0 | % | |
| 125°C,166hr,inUcon®50HB5100,断裂 | ISO 1817 | 9.0 | % | |
| 空气中极限伸长率的变化率 | 23°C,168hr,inMethylethylketone | ASTM D471 | 51 | % |
| 23°C,168hr,inIsopropylAlcohol | ASTM D471 | 28 | % | |
| 23°C,168hr,inHydrochloricAcid,10% | ASTM D471 | 0.0 | % | |
| 质量变化率 | 125°C,168hr,inASTM#1Oil | ASTM D471 | 54 | % |
| 125°C,166hr,inUcon®CC732 | ASTM D471 | 11 | % | |
| 125°C,166hr,inUcon®50HB5100 | ASTM D471 | -19 | % | |
| 125°C,166hr,inSunvis®706Fluid | ASTM D471 | 58 | % | |
| 125°C,166hr,inPydraul®312 | ASTM D471 | 18 | % | |
| 空气中硬度(Shore)的变化率 | ShoreA,23°C,168hr,inSulfuricAcid,98% | ASTM D471 | 0.0 | - |
| ShoreA,23°C,168hr,inSodiumHydroxide,50% | ASTM D471 | 1.0 | - | |
| ShoreA,23°C,168hr,inSodiumChloride,15% | ASTM D471 | 2.0 | - | |
| ShoreA,23°C,168hr,inMethylethylketone | ASTM D471 | 9.0 | - | |
| ShoreA,23°C,168hr,inIsopropylAlcohol | ASTM D471 | 4.0 | - | |
| ShoreA,23°C,168hr,inTrichloroethylene | ASTM D471 | -1.0 | - | |
| ShoreA,100°C,166hr,inASTM#1Oil | ASTM D471 | -12 | - | |
| 硬度 | ShoreA,125°C,166hr,inPydraul®312 | ISO 1817 | -8.0 | - |
| ShoreA,125°C,166hr,inSunvis®706Fluid | ISO 1817 | -15 | - | |
| 空气中硬度(Shore)的变化率 | ShoreA,23°C,166hr,inDioctylPhthalate | ASTM D471 | -1.0 | - |
| ShoreA,23°C,166hr,inDimethylformamide | ASTM D471 | -8.0 | - | |
| ShoreA,23°C,166hr,inDiethylEther | ASTM D471 | -12 | - | |
| ShoreA,23°C,166hr,inBromobenzene | ASTM D471 | -15 | - | |
| ShoreA,23°C,166hr,in1-Propanol | ASTM D471 | 2.0 | - | |
| ShoreA,5°C,166hr,inFreon®11 | ASTM D471 | -15 | - | |
| 硬度 | ShoreA,125°C,166hr,inUcon®50HB5100 | ISO 1817 | 2.0 | - |
| ShoreA,125°C,166hr,inUcon®CC732 | ISO 1817 | -8.0 | - | |
| 空气中极限伸长率的变化率 | 125°C,166hr,inUcon®CC732 | ASTM D471 | -9.0 | % |
| 拉伸应力变化率 | 125°C,166hr,inPydraul®312,断裂 | ISO 1817 | -15 | % |
| 125°C,166hr,inSunvis®706Fluid,断裂 | ISO 1817 | -35 | % | |
| 空气中极限伸长率的变化率 | 125°C,168hr,inASTM#1Oil | ASTM D471 | -43 | % |
| 125°C,168hr,inIRM903Oil | ASTM D471 | -56 | % | |
| 空气中硬度(Shore)的变化率 | ShoreA,23°C,166hr,inZincChloride,10% | ASTM D471 | -2.0 | - |
| ShoreA,23°C,168hr,inAceticAcid | ASTM D471 | -2.0 | - | |
| ShoreA,23°C,168hr,inCyclohexane | ASTM D471 | -16 | - | |
| 质量变化率 | 23°C,166hr,inReferenceFuelC(Isooctane/Toluene,50/50) | ASTM D471 | 69 | % |
| 拉伸应力变化率 | 125°C,70hr,inIRM903Oil,断裂 | ISO 1817 | -48 | % |
| 空气中硬度(Shore)的变化率 | ShoreA,125°C,168hr,inASTM#1Oil | ASTM D471 | -17 | - |
| ShoreA,125°C,168hr,inIRM903Oil | ASTM D471 | -27 | - | |
| ShoreA,125°C,1000hr,inAntifreeze,50/50V/V/Water | ASTM D471 | -4.0 | - | |
| 硬度 | ShoreA,5°C,166hr,inFreon®11 | ISO 1817 | -15 | - |
| ShoreA,23°C,166hr,in1-Propanol | ISO 1817 | 2.0 | - | |
| ShoreA,23°C,166hr,inBromobenzene | ISO 1817 | -15 | - | |
| 拉伸应力变化率 | 125°C,166hr,inAntifreeze,50/50EthyleneGlycol(Prestone®)/Water,断裂 | ISO 1817 | -6.0 | % |
| 空气中极限伸长率的变化率 | 125°C,1000hr,inAntifreeze,50/50V/V/Water | ASTM D471 | -21 | % |
| 拉伸应力变化率 | 5°C,166hr,inFreon®11,断裂 | ISO 1817 | -15 | % |
| 23°C,166hr,in1-Propanol,断裂 | ISO 1817 | 24 | % | |
| 空气中硬度(Shore)的变化率 | ShoreA,23°C,168hr,inDetergent(Tide),2.5% | ASTM D471 | 1.0 | - |
| 质量变化率 | 23°C,168hr,inIsopropylAlcohol | ASTM D471 | -19 | % |
| 5.00°C,166hr,inFreon®11 | ISO 1817 | 140 | % | |
| 体积变化 | 125°C,70hr,在IRM903油中 | ASTM D471 | 97 | % |
| 125°C,70hr,在IRM903油中 | ISO 1817 | 97 | % | |
| 连续使用温度 | 1008hr | SAEJ2236 | 135 | °C |
| 空气中硬度(Shore)的变化率 | ShoreA,23°C,166hr,inReferenceFuelC(Isooctane/Toluene,50/50) | ASTM D471 | -17 | - |
| ShoreA,23°C,166hr,inSeaWater | ASTM D471 | -1.0 | - | |
| ShoreA,23°C,166hr,inTurpentine | ASTM D471 | -16 | - | |
| 拉伸应力变化率 | 125°C,166hr,inAutomaticTransmissionFluid,断裂 | ISO 1817 | -53 | % |
| 125°C,166hr,inPowerSteeringFluid,断裂 | ISO 1817 | -41 | % | |
| 质量变化率 | 23.0°C,166hr,inSeaWater | ISO 1817 | 0.50 | % |
| 23.0°C,168hr,inDetergent(Tide),2.5% | ISO 1817 | 0.90 | % | |
| 23.0°C,166hr,inGlycerol | ISO 1817 | 1.3 | % | |
| 23.0°C,166hr,inDimethylformamide | ISO 1817 | 4.5 | % | |
| 23.0°C,168hr,inSulfuricAcid,98% | ISO 1817 | 4.5 | % | |
| 拉伸应力变化率 | 23°C,168hr,inIsopropylAlcohol,断裂 | ISO 1817 | 28 | % |
| 23°C,168hr,inMethylethylketone,断裂 | ISO 1817 | 51 | % | |
| 质量变化率 | 100°C,166hr,inLithiumGrease | ASTM D471 | 43 | % |
| 100°C,168hr,inDeionizedWater | ASTM D471 | 6.6 | % | |
| 100°C,168hr,inIRM903Oil | ASTM D471 | 92 | % | |
| 23.0°C,166hr,inDiethylEther | ISO 1817 | 13 | % | |
| 拉伸应力变化率 | 23°C,166hr,inGlycerol,断裂 | ISO 1817 | 0.0 | % |
| 23°C,166hr,inHydraulicBrakeFluid,断裂 | ISO 1817 | 3.0 | % | |
| 23°C,166hr,inLithiumGrease,断裂 | ISO 1817 | -9.0 | % | |
| 23°C,166hr,inn-ButylAcetate,断裂 | ISO 1817 | 27 | % | |
| 23°C,166hr,inn-Hexane,断裂 | ISO 1817 | 27 | % | |
| 空气中拉伸强度的变化率 | 23°C,166hr,in1-Propanol | ASTM D471 | 8.0 | % |
| 23°C,166hr,inBromobenzene | ASTM D471 | -30 | % | |
| 125°C,166hr,inPowerSteeringFluid | ASTM D471 | -33 | % | |
| 125°C,166hr,inAntifreeze,50/50EthyleneGlycol(Prestone®)/Water | ASTM D471 | -8.0 | % | |
| 125°C,166hr,inAutomaticTransmissionFluid | ASTM D471 | -46 | % | |
| 23°C,166hr,inDiethylEther | ASTM D471 | 3.0 | % | |
| 125°C,166hr,inPydraul®312 | ASTM D471 | -19 | % | |
| 质量变化率 | 125°C,168hr,inIRM903Oil | ISO 1817 | 99 | % |
| 23.0°C,166hr,inBromobenzene | ISO 1817 | 120 | % | |
| 23°C,168hr,inMethylethylketone | ASTM D471 | -31 | % | |
| 23°C,168hr,inSodiumChloride,15% | ASTM D471 | 0.20 | % | |
| 23°C,168hr,inSodiumHydroxide,50% | ASTM D471 | -0.40 | % | |
| 23°C,168hr,inSulfuricAcid,98% | ASTM D471 | 4.5 | % | |
| 23°C,168hr,inTrichloroethylene | ASTM D471 | -14 | % | |
| 100°C,166hr,inASTM#1Oil | ASTM D471 | 35 | % | |
| 硬度 | ShoreA,100°C,166hr,inLithiumGrease | ISO 1817 | -14 | - |
| 空气中拉伸强度的变化率 | 125°C,70hr,inIRM903Oil | ASTM D471 | -8.0 | % |
| 硬度 | ShoreA,100°C,168hr,inDeionizedWater | ISO 1817 | -2.0 | - |
| ShoreA,100°C,168hr,inIRM903Oil | ISO 1817 | -22 | - | |
| ShoreA,125°C,70hr,inIRM903Oil | ISO 1817 | -23 | - | |
| ShoreA,125°C,166hr,inAntifreeze,50/50EthyleneGlycol(Prestone®)/Water | ISO 1817 | -6.0 | - | |
| ShoreA,125°C,166hr,inAutomaticTransmissionFluid | ISO 1817 | -18 | - | |
| ShoreA,125°C,166hr,inPowerSteeringFluid | ISO 1817 | -20 | - | |
| 空气中极限伸长率的变化率 | 23°C,166hr,inSeaWater | ASTM D471 | 9.0 | % |
| 质量变化率 | 100°C,166hr,inLithiumGrease | ISO 1817 | 43 | % |
| 拉伸应力变化率 | 23°C,166hr,inReferenceFuelA(Isooctane),断裂 | ISO 1817 | -15 | % |
| 空气中硬度(Shore)的变化率 | ShoreA,100°C,168hr,inDeionizedWater | ASTM D471 | -2.0 | - |
| 拉伸应力变化率 | 23°C,168hr,inCyclohexane,断裂 | ISO 1817 | 28 | % |
| 空气中极限伸长率的变化率 | 23°C,166hr,inDioctylPhthalate | ASTM D471 | 21 | % |
| 23°C,166hr,inGlycerol | ASTM D471 | 0.0 | % | |
| 23°C,168hr,inSodiumHydroxide,50% | ASTM D471 | 0.0 | % | |
| 23°C,168hr,inTrichloroethylene | ASTM D471 | 3636 | % | |
| 质量变化率 | 125°C,1000hr,inAntifreeze,50/50V/V/Water | ISO 1817 | 13 | % |
| 125°C,166hr,inPydraul®312 | ISO 1817 | 18 | % | |
| 100°C,166hr,inASTM#1Oil | ISO 1817 | 35 | % | |
| 23.0°C,166hr,inReferenceFuelA(Isooctane) | ISO 1817 | 37 | % | |
| 空气中硬度(Shore)的变化率 | ShoreA,100°C,166hr,inLithiumGrease | ASTM D471 | -14 | - |
| ShoreA,100°C,168hr,inIRM903Oil | ASTM D471 | -22 | - | |
| 拉伸应力变化率 | 23°C,166hr,inSeaWater,断裂 | ISO 1817 | 9.0 | % |
| 23°C,166hr,inTurpentine,断裂 | ISO 1817 | -32 | % | |
| 23°C,166hr,inZincChloride,10%,断裂 | ISO 1817 | 9.0 | % | |
| 23°C,168hr,inAceticAcid,断裂 | ISO 1817 | -8.0 | % | |
| 空气中极限伸长率的变化率 | 23°C,168hr,inSulfuricAcid,98% | ASTM D471 | -18 | % |
| 空气中硬度(Shore)的变化率 | ShoreA,125°C,70hr,inIRM903Oil | ASTM D471 | -23 | - |
| 拉伸应力变化率 | 23°C,166hr,inReferenceFuelC(Isooctane/Toluene,50/50),断裂 | ISO 1817 | -32 | % |
| 空气中拉伸强度的变化率 | 125°C,166hr,inSunvis®706Fluid | ASTM D471 | -30 | % |
| 23°C,168hr,inDetergent(Tide),2.5% | ASTM D471 | -19 | % | |
| 23°C,168hr,inEthanol,95% | ASTM D471 | -7.0 | % | |
| 23°C,168hr,inHydrochloricAcid,10% | ASTM D471 | -9.0 | % | |
| 23°C,168hr,inIsopropylAlcohol | ASTM D471 | 12 | % | |
| 23°C,168hr,inMethylethylketone | ASTM D471 | 31 | % | |
| 23°C,168hr,inSodiumChloride,15% | ASTM D471 | -10 | % | |
| 硬度 | ShoreA,125°C,168hr,inASTM#1Oil | ISO 1817 | -17 | - |
| ShoreA,125°C,168hr,inIRM903Oil | ISO 1817 | -27 | - | |
| ShoreA,125°C,1000hr,inAntifreeze,50/50V/V/Water | ISO 1817 | -4.0 | - | |
| 空气中拉伸强度的变化率 | 23°C,168hr,inSodiumHydroxide,50% | ASTM D471 | -9.0 | % |
| 质量变化率 | 23°C,166hr,inDimethylformamide | ASTM D471 | 4.5 | % |
| 23°C,166hr,inDioctylPhthalate | ASTM D471 | -9.0 | % | |
| 23°C,166hr,inGlycerol | ASTM D471 | 1.3 | % | |
| 23°C,166hr,inHydraulicBrakeFluid | ASTM D471 | 0.20 | % | |
| 硬度 | ShoreA,23°C,168hr,inSodiumChloride,15% | ISO 1817 | 2.0 | - |
| ShoreA,23°C,168hr,inSodiumHydroxide,50% | ISO 1817 | 1.0 | - | |
| 拉伸应力变化率 | 23°C,166hr,inBromobenzene,断裂 | ISO 1817 | -35 | % |
| 23°C,166hr,inDiethylEther,断裂 | ISO 1817 | -3.0 | % | |
| 23°C,166hr,inDimethylformamide,断裂 | ISO 1817 | 3.0 | % | |
| 23°C,166hr,inDioctylPhthalate,断裂 | ISO 1817 | 21 | % | |
| 空气中极限伸长率的变化率 | 23°C,168hr,inSodiumChloride,15% | ASTM D471 | -5.0 | % |
| 硬度 | ShoreA,23°C,166hr,inGlycerol | ISO 1817 | -4.0 | - |
| ShoreA,23°C,166hr,inHydraulicBrakeFluid | ISO 1817 | -3.0 | - | |
| ShoreA,23°C,166hr,inLithiumGrease | ISO 1817 | -7.0 | - | |
| ShoreA,23°C,166hr,inn-ButylAcetate | ISO 1817 | -1.0 | - | |
| ShoreA,23°C,166hr,inn-Hexane | ISO 1817 | -9.0 | - | |
| ShoreA,23°C,166hr,inPyridine | ISO 1817 | 2.0 | - | |
| 空气中极限伸长率的变化率 | 23°C,166hr,inZincChloride,10% | ASTM D471 | 9.0 | % |
| 质量变化率 | 5°C,166hr,inFreon®11 | ASTM D471 | 140 | % |
| 23°C,166hr,in1-Propanol | ASTM D471 | -16 | % | |
| 23°C,166hr,inBromobenzene | ASTM D471 | 120 | % | |
| 空气中极限伸长率的变化率 | 23°C,166hr,inTurpentine | ASTM D471 | -32 | % |
| 空气中拉伸强度的变化率 | 23°C,166hr,inDioctylPhthalate | ASTM D471 | 11 | % |
| 空气中极限伸长率的变化率 | 125°C,166hr,inUcon®50HB5100 | ASTM D471 | 9.0 | % |
| 空气中拉伸强度的变化率 | 23°C,166hr,inGlycerol | ASTM D471 | -5.0 | % |
| 质量变化率 | 23°C,166hr,inSeaWater | ASTM D471 | 0.50 | % |
| 23°C,166hr,inTurpentine | ASTM D471 | 84 | % | |
| 23°C,166hr,inZincChloride,10% | ASTM D471 | 0.40 | % | |
| 拉伸应力变化率 | 23°C,168hr,inSodiumHydroxide,50%,断裂 | ISO 1817 | 0.0 | % |
| 23°C,168hr,inSulfuricAcid,98%,断裂 | ISO 1817 | -18 | % | |
| 23°C,168hr,inTrichloroethylene,断裂 | ISO 1817 | 3636 | % | |
| 100°C,166hr,inASTM#1Oil,断裂 | ISO 1817 | -18 | % | |
| 100°C,166hr,inLithiumGrease,断裂 | ISO 1817 | -26 | % | |
| 100°C,168hr,inDeionizedWater,断裂 | ISO 1817 | -10 | % | |
| 100°C,168hr,inIRM903Oil,断裂 | ISO 1817 | -56 | % | |
| 硬度 | ShoreA,23°C,166hr,inDiethylEther | ISO 1817 | -12 | - |
| ShoreA,23°C,166hr,inDimethylformamide | ISO 1817 | -8.0 | - | |
| ShoreA,23°C,166hr,inDioctylPhthalate | ISO 1817 | -1.0 | - | |
| 质量变化率 | 23.0°C,168hr,inHydrochloricAcid,10% | ISO 1817 | -0.40 | % |
| 23.0°C,166hr,inHydraulicBrakeFluid | ISO 1817 | 0.20 | % | |
| 23.0°C,168hr,inSodiumChloride,15% | ISO 1817 | 0.20 | % | |
| 空气中拉伸强度的变化率 | 23°C,166hr,inDimethylformamide | ASTM D471 | -4.0 | % |
| 23°C,166hr,inHydraulicBrakeFluid | ASTM D471 | -6.0 | % | |
| 23°C,166hr,inLithiumGrease | ASTM D471 | -9.0 | % | |
| 空气中硬度(Shore)的变化率 | ShoreA,125°C,166hr,inUcon®CC732 | ASTM D471 | -8.0 | - |
| 空气中拉伸强度的变化率 | 150°C,168hr | ASTM D573 | -7.0 | % |
| 150°C,168hr | ISO 188 | -7.0 | % | |
| 空气中极限伸长率的变化率 | 150°C,168hr | ASTM D573 | 13 | % |
| 空气中拉伸强度的变化率 | 125°C,166hr,inUcon®50HB5100 | ASTM D471 | -2.0 | % |
| 125°C,166hr,inUcon®CC732 | ASTM D471 | -14 | % | |
| 100°C,168hr,inDeionizedWater | ASTM D471 | -11 | % | |
| 125°C,166hr,inAutomaticTransmissionFluid | ISO 1817 | -46 | % | |
| 125°C,166hr,inPowerSteeringFluid | ISO 1817 | -33 | % | |
| 125°C,166hr,inPydraul®312 | ISO 1817 | -19 | % | |
| 125°C,166hr,inSunvis®706Fluid | ISO 1817 | -30 | % | |
| 质量变化率 | 23.0°C,166hr,inDioctylPhthalate | ISO 1817 | -9.0 | % |
| 23.0°C,168hr,inCyclohexane | ISO 1817 | -3.7 | % | |
| 23.0°C,168hr,inSodiumHydroxide,50% | ISO 1817 | -0.40 | % | |
| 空气中拉伸强度的变化率 | 125°C,166hr,inUcon®50HB5100 | ISO 1817 | -2.0 | % |
| 125°C,166hr,inUcon®CC732 | ISO 1817 | -14 | % | |
| 23°C,168hr,inCyclohexane | ISO 1817 | 15 | % | |
| 23°C,168hr,inDetergent(Tide),2.5% | ISO 1817 | -19 | % | |
| 23°C,168hr,inEthanol,95% | ISO 1817 | -7.0 | % | |
| 质量变化率 | 23.0°C,168hr,inTrichloroethylene | ISO 1817 | -14 | % |
| 23.0°C,166hr,inn-Hexane | ISO 1817 | -13 | % | |
| 空气中拉伸强度的变化率 | 125°C,168hr,inASTM#1Oil | ISO 1817 | -29 | % |
| 质量变化率 | 23.0°C,166hr,inn-ButylAcetate | ISO 1817 | -12 | % |
| 空气中拉伸强度的变化率 | 23°C,168hr,inHydrochloricAcid,10% | ISO 1817 | -9.0 | % |
| 23°C,168hr,inIsopropylAlcohol | ISO 1817 | 12 | % | |
| 23°C,168hr,inMethylethylketone | ISO 1817 | 31 | % | |
| 23°C,168hr,inSodiumChloride,15% | ISO 1817 | -10 | % | |
| 23°C,166hr,inPyridine | ASTM D471 | 2.0 | % | |
| 质量变化率 | 23°C,166hr,inLithiumGrease | ASTM D471 | 12 | % |
| 23°C,166hr,inn-ButylAcetate | ASTM D471 | -12 | % | |
| 23°C,166hr,inn-Hexane | ASTM D471 | -13 | % | |
| 23°C,166hr,inPyridine | ASTM D471 | -16 | % | |
| 硬度 | ShoreA,23°C,168hr,inIsopropylAlcohol | ISO 1817 | 4.0 | - |
| 空气中拉伸强度的变化率 | 23°C,166hr,inSeaWater | ASTM D471 | 3.0 | % |
| 23°C,166hr,inTurpentine | ASTM D471 | -27 | % | |
| 23°C,166hr,inZincChloride,10% | ASTM D471 | 2.0 | % | |
| 硬度 | ShoreA,23°C,168hr,inMethylethylketone | ISO 1817 | 9.0 | - |
| 空气中拉伸强度的变化率 | 23°C,166hr,inReferenceFuelA(Isooctane) | ASTM D471 | -9.0 | % |
| 23°C,166hr,inReferenceFuelC(Isooctane/Toluene,50/50) | ASTM D471 | -25 | % | |
| 23°C,168hr,inAceticAcid | ASTM D471 | -13 | % | |
| 23°C,166hr,inReferenceFuelA(Isooctane) | ISO 1817 | -9.0 | % | |
| 23°C,166hr,inReferenceFuelC(Isooctane/Toluene,50/50) | ISO 1817 | -25 | % | |
| 23°C,166hr,inSeaWater | ISO 1817 | 3.0 | % | |
| 质量变化率 | 23.0°C,166hr,inZincChloride,10% | ISO 1817 | 0.40 | % |
| 空气中硬度变化率 | ShoreA,150°C,168hr | ASTM D573 | 3.0 | - |
| 硬度 | ShoreA,150°C,168hr | ISO 188 | 3.0 | - |
| 空气中拉伸强度的变化率 | 5°C,166hr,inFreon®11 | ASTM D471 | 0.0 | % |
| 23°C,166hr,inTurpentine | ISO 1817 | -27 | % | |
| 拉伸应力变化率 | 23°C,168hr,inSodiumChloride,15%,断裂 | ISO 1817 | -5.0 | % |
| 空气中拉伸强度的变化率 | 23°C,166hr,inZincChloride,10% | ISO 1817 | 2.0 | % |
| 质量变化率 | 23°C,168hr,inAceticAcid | ASTM D471 | 7.0 | % |
| 23°C,168hr,inCyclohexane | ASTM D471 | -3.7 | % | |
| 23°C,168hr,inDetergent(Tide),2.5% | ASTM D471 | 0.90 | % | |
| 23°C,168hr,inEthanol,95% | ASTM D471 | 0.40 | % | |
| 23°C,168hr,inHydrochloricAcid,10% | ASTM D471 | -0.40 | % | |
| 空气中拉伸强度的变化率 | 125°C,168hr,inASTM#1Oil | ASTM D471 | -29 | % |
| 125°C,168hr,inIRM903Oil | ASTM D471 | -43 | % | |
| 125°C,1000hr,inAntifreeze,50/50V/V/Water | ASTM D471 | -7.0 | % | |
| 5°C,166hr,inFreon®11 | ISO 1817 | 0.0 | % | |
| 质量变化率 | 23.0°C,168hr,inEthanol,95% | ISO 1817 | 0.40 | % |
| 空气中极限伸长率的变化率 | 125°C,166hr,inPowerSteeringFluid | ASTM D471 | -41 | % |
| 125°C,166hr,inPydraul®312 | ASTM D471 | -15 | % | |
| 125°C,166hr,inSunvis®706Fluid | ASTM D471 | -35 | % | |
| 150°C,168hr | ISO 188 | 13 | % | |
| 空气中拉伸强度的变化率 | 100°C,168hr,inIRM903Oil | ASTM D471 | -40 | % |
| 空气中极限伸长率的变化率 | 23°C,166hr,inBromobenzene | ASTM D471 | -35 | % |
| 23°C,166hr,inDiethylEther | ASTM D471 | -3.0 | % | |
| 23°C,166hr,inDimethylformamide | ASTM D471 | 3.0 | % | |
| 空气中拉伸强度的变化率 | 23°C,168hr,inSodiumHydroxide,50% | ISO 1817 | -9.0 | % |
| 23°C,168hr,inAceticAcid | ISO 1817 | -13 | % | |
| 23°C,168hr,inSulfuricAcid,98% | ASTM D471 | -5.0 | % | |
| 100°C,166hr,inASTM#1Oil | ASTM D471 | -13 | % | |
| 100°C,166hr,inLithiumGrease | ASTM D471 | -25 | % | |
| 125°C,168hr,inIRM903Oil | ISO 1817 | -43 | % | |
| 125°C,1000hr,inAntifreeze,50/50V/V/Water | ISO 1817 | -7.0 | % | |
| 空气中极限伸长率的变化率 | 5°C,166hr,inFreon®11 | ASTM D471 | -15 | % |
| 23°C,166hr,in1-Propanol | ASTM D471 | 24 | % | |
| 空气中拉伸强度的变化率 | 23°C,168hr,inSulfuricAcid,98% | ISO 1817 | -5.0 | % |
| 100°C,166hr,inASTM#1Oil | ISO 1817 | -13 | % | |
| 100°C,166hr,inLithiumGrease | ISO 1817 | -25 | % | |
| 100°C,168hr,inDeionizedWater | ISO 1817 | -11 | % | |
| 23°C,168hr,inCyclohexane | ASTM D471 | 15 | % | |
| 125°C,166hr,inAntifreeze,50/50EthyleneGlycol(Prestone®)/Water | ISO 1817 | -8.0 | % | |
| 100°C,168hr,inIRM903Oil | ISO 1817 | -40 | % | |
| 125°C,70hr,inIRM903Oil | ISO 1817 | -8.0 | % | |
| 质量变化率 | 125°C,166hr,inPowerSteeringFluid | ISO 1817 | 72 | % |
| 拉伸应力变化率 | 23°C,168hr,inEthanol,95%,断裂 | ISO 1817 | 3.0 | % |
| 空气中拉伸强度的变化率 | 23°C,166hr,inn-ButylAcetate | ASTM D471 | 16 | % |
| 23°C,166hr,inn-Hexane | ASTM D471 | 14 | % | |
| 空气中极限伸长率的变化率 | 23°C,166hr,inLithiumGrease | ASTM D471 | -9.0 | % |
| 23°C,166hr,inn-ButylAcetate | ASTM D471 | 27 | % | |
| 23°C,166hr,inn-Hexane | ASTM D471 | 27 | % | |
| 空气中拉伸强度的变化率 | 23°C,166hr,inHydraulicBrakeFluid | ISO 1817 | -6.0 | % |
| 23°C,166hr,inLithiumGrease | ISO 1817 | -9.0 | % | |
| 23°C,166hr,inn-ButylAcetate | ISO 1817 | 16 | % | |
| 23°C,166hr,inn-Hexane | ISO 1817 | 14 | % | |
| 23°C,166hr,inPyridine | ISO 1817 | 2.0 | % | |
| 23°C,166hr,in1-Propanol | ISO 1817 | 8.0 | % | |
| 23°C,166hr,inBromobenzene | ISO 1817 | -30 | % | |
| 23°C,166hr,inDiethylEther | ISO 1817 | 3.0 | % | |
| 23°C,166hr,inDimethylformamide | ISO 1817 | -4.0 | % | |
| 23°C,166hr,inDioctylPhthalate | ISO 1817 | 11 | % | |
| 23°C,166hr,inGlycerol | ISO 1817 | -5.0 | % | |
| 质量变化率 | 125°C,166hr,inAntifreeze,50/50EthyleneGlycol(Prestone®)/Water | ASTM D471 | 6.8 | % |
| 125°C,168hr,inASTM#1Oil | ISO 1817 | 54 | % | |
| 125°C,166hr,inSunvis®706Fluid | ISO 1817 | 58 | % | |
| 125°C,166hr,inAutomaticTransmissionFluid | ISO 1817 | 62 | % | |
| 23.0°C,166hr,inReferenceFuelC(Isooctane/Toluene,50/50) | ISO 1817 | 69 | % | |
| 23.0°C,166hr,inTurpentine | ISO 1817 | 84 | % | |
| 100°C,168hr,inIRM903Oil | ISO 1817 | 92 | % | |
| 拉伸应力变化率 | 23°C,168hr,inDetergent(Tide),2.5%,断裂 | ISO 1817 | -15 | % |
| 23°C,168hr,inHydrochloricAcid,10%,断裂 | ISO 1817 | 0.0 | % | |
| 硬度 | ShoreA,23°C,168hr,inSulfuricAcid,98% | ISO 1817 | 0.0 | - |
| ShoreA,23°C,168hr,inTrichloroethylene | ISO 1817 | -1.0 | - | |
| ShoreA,100°C,166hr,inASTM#1Oil | ISO 1817 | -12 | - | |
| 空气中极限伸长率的变化率 | 23°C,166hr,inHydraulicBrakeFluid | ASTM D471 | 3.0 | % |
| 23°C,166hr,inPyridine | ASTM D471 | 21 | % | |
| 23°C,166hr,inReferenceFuelA(Isooctane) | ASTM D471 | -15 | % | |
| 23°C,166hr,inReferenceFuelC(Isooctane/Toluene,50/50) | ASTM D471 | -32 | % | |
| 空气中硬度(Shore)的变化率 | ShoreA,23°C,166hr,inGlycerol | ASTM D471 | -4.0 | - |
| ShoreA,23°C,166hr,inHydraulicBrakeFluid | ASTM D471 | -3.0 | - | |
| ShoreA,23°C,166hr,inLithiumGrease | ASTM D471 | -7.0 | - | |
| 质量变化率 | 125°C,168hr,inIRM903Oil | ASTM D471 | 99 | % |
| 125°C,1000hr,inAntifreeze,50/50V/V/Water | ASTM D471 | 13 | % | |
| 23.0°C,168hr,inMethylethylketone | ISO 1817 | -31 | % | |
| 空气中极限伸长率的变化率 | 125°C,166hr,inAutomaticTransmissionFluid | ASTM D471 | -53 | % |
| 拉伸应力变化率 | 125°C,1000hr,inAntifreeze,50/50V/V/Water,断裂 | ISO 1817 | -21 | % |
| 质量变化率 | 23.0°C,168hr,inIsopropylAlcohol | ISO 1817 | -19 | % |
| 125°C,166hr,inUcon®50HB5100 | ISO 1817 | -19 | % | |
| 23.0°C,166hr,inPyridine | ISO 1817 | -16 | % | |
| 23.0°C,166hr,in1-Propanol | ISO 1817 | -16 | % | |
| 空气中极限伸长率的变化率 | 100°C,166hr,inASTM#1Oil | ASTM D471 | -18 | % |
| 100°C,168hr,inIRM903Oil | ASTM D471 | -56 | % | |
| 125°C,70hr,inIRM903Oil | ASTM D471 | -48 | % | |
| 125°C,166hr,inAntifreeze,50/50EthyleneGlycol(Prestone®)/Water | ASTM D471 | -6.0 | % | |
| 100°C,168hr,inDeionizedWater | ASTM D471 | -10 | % | |
| 空气中硬度(Shore)的变化率 | ShoreA,125°C,166hr,inAntifreeze,50/50EthyleneGlycol(Prestone®)/Water | ASTM D471 | -6.0 | - |
| ShoreA,125°C,166hr,inAutomaticTransmissionFluid | ASTM D471 | -18 | - | |
| ShoreA,125°C,166hr,inPowerSteeringFluid | ASTM D471 | -20 | - | |
| ShoreA,125°C,166hr,inPydraul®312 | ASTM D471 | -8.0 | - | |
| 空气中极限伸长率的变化率 | 100°C,166hr,inLithiumGrease | ASTM D471 | -26 | % |
| 空气中硬度(Shore)的变化率 | ShoreA,125°C,166hr,inSunvis®706Fluid | ASTM D471 | -15 | - |
| ShoreA,125°C,166hr,inUcon®50HB5100 | ASTM D471 | 2.0 | - | |
| 质量变化率 | 23°C,166hr,inReferenceFuelA(Isooctane) | ASTM D471 | 37 | % |
| 100°C,168hr,inDeionizedWater | ISO 1817 | 6.6 | % | |
| 125°C,166hr,inAntifreeze,50/50EthyleneGlycol(Prestone®)/Water | ISO 1817 | 6.8 | % | |
| 23.0°C,168hr,inAceticAcid | ISO 1817 | 7.0 | % | |
| 125°C,166hr,inUcon®CC732 | ISO 1817 | 11 | % | |
| 23.0°C,166hr,inLithiumGrease | ISO 1817 | 12 | % | |
| 拉伸应力变化率 | 23°C,166hr,inPyridine,断裂 | ISO 1817 | 21 | % |
| 硬度 | ShoreA,23°C,166hr,inSeaWater | ISO 1817 | -1.0 | - |
| ShoreA,23°C,166hr,inTurpentine | ISO 1817 | -16 | - | |
| 质量变化率 | 23°C,166hr,inDiethylEther | ASTM D471 | 13 | % |
| 硬度 | ShoreA,23°C,166hr,inZincChloride,10% | ISO 1817 | -2.0 | - |
| ShoreA,23°C,168hr,inAceticAcid | ISO 1817 | -2.0 | - | |
| ShoreA,23°C,168hr,inCyclohexane | ISO 1817 | -16 | - | |
| ShoreA,23°C,168hr,inDetergent(Tide),2.5% | ISO 1817 | 1.0 | - | |
| ShoreA,23°C,168hr,inEthanol,95% | ISO 1817 | 0.0 | - | |
| ShoreA,23°C,168hr,inHydrochloricAcid,10% | ISO 1817 | 1.0 | - | |
| ShoreA,23°C,166hr,inReferenceFuelA(Isooctane) | ISO 1817 | -13 | - | |
| ShoreA,23°C,166hr,inReferenceFuelC(Isooctane/Toluene,50/50) | ISO 1817 | -17 | - | |
| 质量变化率 | 125°C,166hr,inAutomaticTransmissionFluid | ASTM D471 | 62 | % |
| 125°C,166hr,inPowerSteeringFluid | ASTM D471 | 72 | % | |
| 空气中极限伸长率的变化率 | 23°C,168hr,inAceticAcid | ASTM D471 | -8.0 | % |
| 23°C,168hr,inCyclohexane | ASTM D471 | 28 | % | |
| 23°C,168hr,inEthanol,95% | ASTM D471 | 3.0 | % | |
| 23°C,168hr,inDetergent(Tide),2.5% | ASTM D471 | -15 | % |